Abstract:1,3-diglycidyl-5,5-dimethyl hydantoin(DGDH) was cured with phthalic anhydride(PA) and polysebacic polyanhydride(PSPA).The reaction kinetics and heat stabilization,in the curing process were studied using DSC and TGA respectively.The DGDH/PA system was modified using the curing agent PSPA with different proportions.Tensile strength,fracture toughness,heat deflection temperature and morphology of fracture surface were characterized.Kinetic results show that DGDH/PSPA has activation energy of 75.94 kJ/mol,while that of DGD/PSPA is only 56.25 kJ/mol.The heat stabilization of DGDH/PA is worse than that of DGDH/PSPA,when 34% of PSPA was added into DGDH/PA system,the fracture toughness is improved from 2.16 kJ/m2 for the unmodified system to 6.45 kJ/m2 for the modified system,however,the heat deflection temperature decreases from 132.2 ℃ to 51.8 ℃,accordingly.Comparing with the unmodified system,the modified system has irregular tracks of crack propagation,which attributes to the improvement of fracture toughness.