Abstract:With 2,2-bis [4-(4-amino-phenoxy)phenyl]propane(BAPP),p-phenylenediamine(PDA) and 4,4 '- biphenyl dianhydride(BPDA) as main raw materials, polyamic acid(PAA) resin was synthesized by copolymerization. Then,PAA resin was coated on the surface of electrolytic copper foil and imidized at high temperature under high purity nitrogen protection. A flat, smooth and flexible polyimide copper clad laminate was finally prepared. The properties of PI copper clad laminate with different molar ratio of BAPP/PDA,pre-curing process and thermal imidization process of PAA resin, winding traction of coating machine were studied. The results show that PI copper clad laminate with better comprehensive properties was prepared with the molar ratio of BAPP/PDA 1.5/4.5,under the pre-curing process of PAA resin, such as the coating speed is 0.6m/min, the length of the drying tunnel is 9m, the temperature distribution of drying tunnel is 110 ℃,140 ℃,170 ℃,the thermal imidization process is 200 ℃/1h,250 ℃/1h,320 ℃/2h and winding traction is 14kg~16kg.