An environmental friendly resin adhesive was prepared using mix sugar instead of formaldehyde under alkaline condition. The adhesive force was used as an index to investigate and optimize reactive conditions by the response surface methodology (RSM). By analyzing and comparing the experimental result, the optimum conditions of the reaction process were gained: the catalyst amount is 6.9%, the reaction temperature is 79 ℃, the reaction time is 6.02 h and the mole ratio of mix sugar and urea is 5.02∶1. Under these conditions, the theoretical adhesive force of the products is 457.292N and the measured value is 456.49N.