Abstract:In this paper, wood fibers were classified into four groups (120 mesh~80 mesh, 80 mesh~40 mesh, 40 mesh~20 mesh, and 20 mesh~10 mesh). The performance of wood fiber reinforced high density polyethylene (HDPE) composites after experiencing ultraviolet (UV) accelerated aging was investigated. The results show that the composite reinforced with 20 mesh~10 mesh wood fiber possesses the best flexural performance, however, its impact strength is the worst. Bending strength and modulus of elasticity of these composites decrease by 18% and 34%, respectively, after exposing to 2000 h UV accelerated aging. The impact strength of all composites increases during accelerated aging. Composite filled with 20 mesh~10 mesh wood fibers obtain the highest impact strength. SEM analysis shows small cracks on the weathered surface of composites, and composites with 20 mesh~10 mesh wood fibers are most severely damaged. FT IR indicates oxidation occurred on the surface during aging, however, condensation affects the detection to surface oxidation.