Abstract:Using Ba(OH)2·8H2O as catalyst, low free formaldehyde barium phenolic foam resin was synthesized by gradually warming dropping. The effect of different mole ratio of F/P, catalyst amount, reaction time, reaction temperature on the free phenol and methylol content of foaming barium phenolic foam resin was explored. The appropriate synthetic processes was determined, such as the mole ratio of F/P 1∶1.3 to 1.6, the reaction temperature 80 ℃ to 85 ℃, reaction time 2h, the catalyst amount of 5%. The free phenol content of final barium phenolic foam resin is 3%, carbon residue is 44.3%, solid content is from 78% to 85%, the oxygen index (LOI) is 54.9, analyzed by FT-IR and TG characterization.