Abstract:A series of poly(amic acid)s(PAAs) containing diphenylpyridine were synthesized from the reaction of 3,3′,4,4′-biphenyl tetracarboxylic dianhydride with 4,4-oxydianiline(ODA) and 2,5-bis(4-aminophenyl)pyridine (PRD), followed by coating these PAAs solutions onto copper foils and then imidizing thermally. The dimensional stability and peel strength of the resulting two-layer flexible copper-clad laminates were characterized. It is found that when the mole ratio of PRD to ODA is 1∶1, the coefficient of thermal expansion (CTE) values of the polyimide (PI) is close to the value of the copper foil, and the 90°-peel strength of the laminate reaches the maximum value of 19.7 N/cm. Hence, the physical properties of polyimide containing PRD could match simultaneously requirement of curl-free polyimide/copper laminate in dimensional stability and adhesion properties.