Abstract:Polyacrylamide/ polyacrylate sodium double network hydrogel was synthesized by two-step free radical polymerization, using laponite as crosslinker in polyacrylamide (PAM) network and N,N’-methylenebisacrylamide (BIS) as crosslinker in polyacrylic acid (PAA) network. The tensile strength of the double hydrogel can reach about 137 kPa with nimble pH response. The tensile properties and response performance were adjusted by changing the neutralization degree of AA, the crosslinker amount and monomer ratio. The results show that the best tensile strength is up to 137 kPa when the neutralization degree of AA is 125%, m(AM)∶m(K2S2O8)=1∶0.002, m(AM)∶m(Laponite)=1∶0.6, m(AA)∶m(BIS)=1∶0.002, m(AM)∶m(AA)=1∶7. Also, the double hydrogel has a nimble and reversible pH response, and is shrunk in the medium of pH<4 and is swelled in the medium of pH>5.