Abstract:The hexagonal boron nitride(h-BN) modified with the coupling agent then was filled in methyl vinyl silicone rubber(MVQ) by melt blending using a internal mixer and a two roll mixing mill, and then samples were prepared by compression molding. Elastic modulus, cure characteristic, morphology, thermally conductive property and dielectric constant were characterized by rubber process analyzer(RPA), scanning electron microscopy (SEM), thermal conductivity analysis instrument and impedance analyzer. The results show that Payne effect appears at the amount of 20 phr h-BN. The elastic modulus, vulcanization time, thermal conductivity and the dielectric constant increase with increasing h-BN amount; but with the increasing h-BN amount, the scorch time and curing time is shortened. When the h-BN amount is 50 phr, the thermal conductivity and dielectric constant of h-BN/MVQ composites are 1.13 W/(m·K) and 3.87 respectively, the comprehensive performance is better.