Abstract:This work was aimed to explore the effect of different drying temperatures on the morphology, crystallization, thermal stability, transparency, mechanical and barrier properties of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH) films, which was prepared by solution casting method with N,N-dimethylformamide (DMF) as solvent, by corresponding test methods. The results show that as the temperature rises, the densification, crystallinity, thermal stability, elongation at break and barrier properties of PHBH films increase firstly and then decrease, with the decrease of grain size and gradually, and the increase of transparency and tensile strength. When the drying temperature is 55 ℃, the PHBH film has a smooth cross section, good crystallinity, thermal stability, mechanical strength and barrier property. The tensile strength and the elongation at break are 20.26 MPa and 25% respectively, and the oxygen and water vapor transmittance are 5.7×10-15cm3·cm/(cm2·s·Pa) and 2.21×10-14 g·cm/(cm2·s·Pa), respectively.