Abstract:Aramid III fibers were modified with a mixture of water-soluble epoxy resin (PAEK) and thermoplastic polyacrylamide (APAM) to investigate the storage stability, centrifugal stability, surface tension, viscosity and particle size of the slurry. And the surface functional groups of the slurry were analyzed, and then studied the effect of slurry concentration on the fiber strength. Through SEM, ATR-FT-IR, X-ray and XPS, the surface morphology and chemical composition of fibers after sizing were characterized. The results show that the prepared slurry has a small particle size, uniform dispersion and good stability. SEM, XPS, and ATR-FT-IR measurements show that the surface of aramid III fibers becomes rough after sizing, and the number of polar functional groups on the surface of fibers increases; when the sizing concentration is 3%, compared with the untreated aramid III, the tensile strength of aramid III monofilament increases by 7.95%, and the tensile strength of bundle filaments is increased by 14.16%.