Abstract:Erucylamide was added into styrene-butadiene rubber (SBR)/butadiene rubber (BR) at different contents, and the properties of the rubber compounds were characterized by vulcanization characteristics, mechanical properties and friction coefficient. The results show that when the dosage of erucylamide is 2~10 phr, the friction coefficient of vulcanizate decreases gradually, and the elongation at break and flexural energy increase gradually. When the amount of erucylamide in vulcanizate is 10 phr, compared with the group without erucylamide, the hardness, compression set, static friction coefficient, dynamic friction coefficient and tensile strength are decreased by 9.21%, 51.61%, 45.51%, 37.54% and 19.84%, respectively and the elongation at break and the flexible number are increased by 36.14% and 88.92%, respectively. Through the analyses of RPA and SEM, these results are related to the addition of erucylamide to improve the dispersibility of fillers.