Abstract:Thermoset polyimides with multiple molecular weight were synthesized by PMR using 4-phenylacetylene phthalic anhydride as reactive end sealing agent, 2,3,3',4'-diphthalic anhydride (α-BPDA) and 4,4'-diaminodiphenyl ether (4,4'-ODA) as dihydride and diamine monomers. DSC, DMA, TGA and rheology were used to study the relationship between molecular weight and curing reaction characteristics, rheological properties, heat resistance, toughness and its influence mechanism. The results indicate that with the increase of molecular weight, the minimum viscosity of the melt is increased from 10.4 Pa·s to 1449.4 Pa·s, the glass transition temperature is decreased from 369 ℃ to 346 ℃, and the impact strength is increased from 31.69 kJ/m2 to 62.15 kJ/m2. By optimizing the molecular weight, the comprehensive control of toughness, heat resistance and process performance can be achieved.